Guangzhou Steel News: slab steel welding crack control measures

Time:[2015-5-30]  Hits:5240

Guangzhou Steel News: slab steel welding crack control measures


   A large slab of steel components, steel thick weld deposit large, complex nodes, residual stress, prone to crack, affecting the quality of welding, which is important and difficult project quality control. Production of general measures are:

1, measures to prevent hot cracking
1) Control of the chemical composition of the weld. I.e. to reduce the low-melting eutectic composition readily segregation elements, such as sulfur and phosphorus content in the welding material and the base material is formed. Reduce the carbon content in the steel, can reduce the thermal cracking tendencies; improve Mn content can improve weld thermal cracking performance.
2) control of welding parameters and conditions. Control of welding current and welding speed, so that the aspect ratio of each cross section of the upper part of bead reach 1.1 to 1.2, can improve thermal cracking performance, while controlling the weld pool shape, do not form easily understood in sharp elongated bath a longitudinal weld surface thermal cracks. Preheat reduces tendency to form cracks; reasonable welding sequence can make the most of the weld at the smaller restraint of welding, reducing the tensile stress suffered weld shrinkage, thermal cracking tendency can be reduced.
2, cold cracking prevention measures
1) Before welding procedure qualification test performed to determine the process parameters.
2) preheat prevents cracking, as well as improve the performance of a certain action.
3) manual welding using low hydrogen electrodes alkaline E5Q / E55 type; CO: gas shielded arc welding flux cored wire can be used; a H08MnA submerged arc welding can be used F5021, and in strict accordance with the provisions drying. Drying temperature is 350-450 ℃, after dried at 100-150cC temperature for 1 ~ 2h, put insulation cylinder used with the check.
4) Choose a reasonable weld profile, in strict accordance with the drawings machining parts groove.
5) each side of the weld within the range of 30 ~ 50mm rust and water clean, reducing the source of hydrogen.
6) cracks often occur on the head welds and weld root, so tacking length, welding foot height and spacing should also make corresponding provisions. If you have to locate the weld in the groove proceeds, weld height should be less than 2/3 of the groove depth, the length should be greater than 40mm. If necessary, prior to tack welding is preheated. Before welding, positioning the weld inspection, it must be removed when re-welding cracks. Tack welding length and spacing, should be considered the base material thickness, structure length.
7) To reduce stress and prevent cracking during welding, the assembly should avoid forced assembly.
8) appropriate to increase the current, lower cooling rate, helps prevent the formation of hardened tissue.
9) Control interlayer temperature should be slightly higher preheat temperature.
10) Q345C soldering should be carried out after a slow cooling to slow cooling rate of the weld and heat affected zone and prevent cold cracking, respond promptly weldment insulation, that is immediately after welding weldment is heated to 250 to 350. And use of asbestos and other insulation 2.6h after air cooling can reduce the hydrogen content in the weld and prevent cold cracking, heating methods, with preheat before width.
While slab steel construction difficult, but as long as proper control measures, the proportion of component cracking will be greatly reduced, the project will significantly improve the quality of weld cracks will be avoided, it can effectively control the quality of construction industry. Guangzhou Steel

Copyright:佛山市勝邦鋼結構有限公司 Foshan Shengbang Steel Structure Co., Ltd. Record Number:粵ICP備13078463號
欧美最猛性久久久久久| 伊人久久一次| 国产成人av乱码在线观看| 综合色区中文字幕首页亚洲| 亚洲日本精品熟女视频| 亚洲国产网友自拍| 91人妻视频| 国产最新超清理论在线| 丁香激情亚洲| 一色屋精品亚洲香蕉网站| 乱码人妻Av一区二区三区| 嫩草嫩草嫩草影院| 日韩国产欧美视频一区二区三区| 99在线视频观看| 自慰欧美在线看| 久99久精品视频网| 久久一级5| 国产欧美日韩剧情| 欧美日韩国产Ⅴa在线观看免费| 国产伦精品一区二区三区竹菊| 禄劝| 色狼人av| 欧美理论一级| 色哟哟国产精品一区二区| 伊人丁香中文字幕| 久久久精品三级无码| 日韩人妻在线免费观看| 午夜夜操天天干| 亚洲AV成人无码AV小说| 干日韩少妇av| 久久久久久国产精品免费西安| 欧美妇女在线| 中文精品在线| 亚洲国产精品自产拍久久| 精品无码av毛片一区二区三区| 秘国产成人免费网站| 老色鬼久久亚洲av综合| 少妇肥臀一区二区三区| 久久成人国产精品一区二区| 国产怡红院在线| 中国日本熟妇|